详细介绍: (1)选用直流等离子粉末堆焊机,电流为200A—280A,电压为22V—28V;(2)所用夹紧钻杆接头装置能够在焊枪下正、反旋转钻杆接头,转速可调;(3)夹紧焊枪并带动焊枪摆动,摆频为30一90mm,可调,摆幅为15—40mm,可调; (4)焊枪上、下、左、右均可大范围移动; (5)焊机送粉机构运行要平稳,速度可调,压丝轮压紧度适中,可调,送粉速度为6—12mm每分钟,可调。
2.敷焊工艺 针对镍基耐磨带我们探索出一套敷焊工艺参数:焊接电流230—280A、送粉速度6—8mm每分钟、焊机摆频40一50每分钟、敷焊速度120—130mm每分钟、敷焊距离8mm—12mm、敷焊角90°和保护气流量5—8L每分钟。按以上焊接参数敷焊,新型耐磨带合金焊粉敷焊质量可达到以下技术要求: (1)焊接过程稳定,送丝平稳; (2)耐磨带尺寸符合标准要求,宽度30一35mm,高度2mm;(3)耐磨带表面鱼鳞状花纹均匀、致密、平整、光滑;(4)耐磨带表面无过多残渣、飞溅,无咬边现象,边缘齐整;(5)耐磨带与基体熔合较好,无较大裂纹和针孔。
![](http://img05.jdzj.com/oledit/UploadFile/news2014c/image/20150114/20150114141948124812.jpg) ![](http://img05.jdzj.com/oledit/UploadFile/news2014c/image/20150114/20150114141978397839.jpg) ![](http://img05.jdzj.com/oledit/UploadFile/news2014c/image/20150114/20150114141999389938.jpg) ![](http://img05.jdzj.com/oledit/UploadFile/news2014c/image/20150114/20150114141960826082.jpg) ![](http://img05.jdzj.com/oledit/UploadFile/news2014c/image/20150114/20150114141987798779.jpg) ![](http://img05.jdzj.com/oledit/UploadFile/news2014c/image/20150114/20150114141931423142.jpg) |